Effect of Multi-Stand Pipe Mill Rolling and Sizing Process on Structure and Property of N80 Non-Quenching and Tempering Steel 36-40Mn2V for Oil Well Pipe
|更新时间:2026-01-21
|
Effect of Multi-Stand Pipe Mill Rolling and Sizing Process on Structure and Property of N80 Non-Quenching and Tempering Steel 36-40Mn2V for Oil Well Pipe
Special SteelVol. 33, Issue 3, Pages: 53-56(2012)
作者机构:
1. 武汉科技大学钢铁冶金及资源利用省部共建教育部重点实验室,武汉,430081
2. 衡阳华菱钢管(集团)有限公司,衡阳,421001
作者简介:
基金信息:
DOI:
CLC:
Received:15 November 2011,
Online First:14 October 2022,
Published:14 October 2012
稿件说明:
移动端阅览
方剑, 李阳华, 邹喜洋, et al. Effect of Multi-Stand Pipe Mill Rolling and Sizing Process on Structure and Property of N80 Non-Quenching and Tempering Steel 36-40Mn2V for Oil Well Pipe[J]. Special Steel, 2012, 33(3): 53-56.
DOI:
方剑, 李阳华, 邹喜洋, et al. Effect of Multi-Stand Pipe Mill Rolling and Sizing Process on Structure and Property of N80 Non-Quenching and Tempering Steel 36-40Mn2V for Oil Well Pipe[J]. Special Steel, 2012, 33(3): 53-56.DOI:
Effect of Multi-Stand Pipe Mill Rolling and Sizing Process on Structure and Property of N80 Non-Quenching and Tempering Steel 36-40Mn2V for Oil Well Pipe
The effect of 340 multi-stand pipe mill (MPM) continuous rolling process (at 950 ~ 1 100 °C with strain 0. 5 ~ 0. 8
strain rate 1. 0 s _ 1
water or 3 °C/s cooling) and sizing process ( at 800 ~ 950 °C
with strain 0. 1 ~ 0. 3
strain rate 0. 5 s
-1
air cooiing) on structure
and hardness of steel 36Mn2V and 40Mn2V has been simulated by using Gleeble-1500 thermal simulation machine. Results show that with MPM deformation temperature being higher than 1 050 °C at strain 0. 5
the complete dynamic recrystallization of steel 36Mn2V and 40Mn2V occurs
the grains are fine and the comprehensive properties are improved; As sizing strain of steel 36Mn2V is 0. 3 and sizing strain of steel 40Mn2V is 0. 2
as the sizing temperature is controlled higher than 835 °C