Test on Increasing Drop Strength of Complex Deoxidizer by Epoxy Resin Binder and Application
|更新时间:2026-01-21
|
Test on Increasing Drop Strength of Complex Deoxidizer by Epoxy Resin Binder and Application
Special SteelVol. 37, Issue 3, Pages: 5-7(2016)
作者机构:
辽宁科技大学材料与冶金学院,鞍山,114051
作者简介:
基金信息:
DOI:
CLC:
Received:20 December 2015,
Online First:02 August 2022,
Published:02 August 2016
稿件说明:
移动端阅览
亢淑梅, 于长鸿, 沈明钢, et al. Test on Increasing Drop Strength of Complex Deoxidizer by Epoxy Resin Binder and Application[J]. Special Steel, 2016, 37(3): 5-7.
DOI:
亢淑梅, 于长鸿, 沈明钢, et al. Test on Increasing Drop Strength of Complex Deoxidizer by Epoxy Resin Binder and Application[J]. Special Steel, 2016, 37(3): 5-7.DOI:
Test on Increasing Drop Strength of Complex Deoxidizer by Epoxy Resin Binder and Application
According the issue of Al-CaO complex deoxidizer for clean steel easily crushing during process of falling from 10 meters high burden bin led to low utilization
increase of cost and dust pollution in situ
the effect of adding epoxy resin
modified starch etc binders with 0-2.5% content in Al-CaO complex deoxider fine powder and binder curing at 180-350 °C on drop strength of complex deoxidizer has been studied. Results show that the epoxy resin is better than modified starch
with increasing epoxy resin content the drop strength of complex deoxidizer increases
and as the epoxy resin content is more than 2.0%
the crushing rate is no-obvious change; with adding 2.0% epoxy resin and curing at 350℃
the crushing rate of complex deoxidizer is minimum that is 17.5%. The application o£ adding epoxy resin in Al-CaO complex deoxidizer for EH40 steel in RH refining show that with adding epoxy resin the drop strength of complex deoxidizer increases obviously to decrease the dust pollution in situ and the cost for control pollution.