Dephosphorization Study on 60 t Converter Slagging by Limestone Replacing Lime as Slagging Material
|更新时间:2026-01-21
|
Dephosphorization Study on 60 t Converter Slagging by Limestone Replacing Lime as Slagging Material
Special SteelVol. 37, Issue 3, Pages: 28-30(2016)
作者机构:
1. 山西工程职业技术学院冶金工程系,太原,030009
2. 北京科技大学冶金与生态工程学院,北京,100083
作者简介:
基金信息:
DOI:
CLC:
Received:15 December 2015,
Online First:02 August 2022,
Published:02 August 2016
稿件说明:
移动端阅览
郝赳赳, 李宏, 胡龙飞, et al. Dephosphorization Study on 60 t Converter Slagging by Limestone Replacing Lime as Slagging Material[J]. Special Steel, 2016, 37(3): 28-30.
DOI:
郝赳赳, 李宏, 胡龙飞, et al. Dephosphorization Study on 60 t Converter Slagging by Limestone Replacing Lime as Slagging Material[J]. Special Steel, 2016, 37(3): 28-30.DOI:
Dephosphorization Study on 60 t Converter Slagging by Limestone Replacing Lime as Slagging Material
The dephosphorizing effect of 60 t converter on 0. 03% ~ 0.27% C
0. 012% ~ 0. 024% P
0. 023% ~ 0. 036% S liquid at 1580 ~ 1680 ℃. by limestone replacing lime as slag material is tested and studied to compare the slagsteel phosphor partition ratio by limestone as slagging material with that by lime as slagging material
and to get the effect of TFe in slag
end slag basicity and liquid end temperature by limestone as slag material on slag-steel phosphor partition ratio- Lp. The results show that by limestone replacing lime as slagging material the mode of oxidizing of iron and phosphor in liquid and the dephosphorizing reaction way are same
but the dephosphorizing effect of liquid is better
that is by lime as slagging material the average Lp is 80
while by limestone as slagging material the average Lp is 101. By limestone replacing lime as slagging material the effect of dephosphorizing is best with TFe in slag 14% 〜17%
end slag basicity 3.1〜3. 4 and liquid end temperature 1600 ~1630 ℃.