Water Model Study on Effect of Process Parameters on Top and Bottom Combined Blowing of 120 t BOF and Application
|更新时间:2026-01-21
|
Water Model Study on Effect of Process Parameters on Top and Bottom Combined Blowing of 120 t BOF and Application
Special SteelVol. 38, Issue 1, Pages: 1-3(2017)
作者机构:
辽宁科技大学材料与冶金学院,鞍山,114051
作者简介:
基金信息:
DOI:
CLC:
Received:01 August 2016,
Online First:28 July 2022,
Published:28 July 2017
稿件说明:
移动端阅览
韩楚菲, 沈明钢, 杨晨. Water Model Study on Effect of Process Parameters on Top and Bottom Combined Blowing of 120 t BOF and Application[J]. Special Steel, 2017, 38(1): 1-3.
DOI:
韩楚菲, 沈明钢, 杨晨. Water Model Study on Effect of Process Parameters on Top and Bottom Combined Blowing of 120 t BOF and Application[J]. Special Steel, 2017, 38(1): 1-3.DOI:
Water Model Study on Effect of Process Parameters on Top and Bottom Combined Blowing of 120 t BOF and Application
研究氧枪距离熔池高度(200~280 mm)、顶氧枪流量(72.5~99.0 m3/h)、底吹流量(0.8~2.4 m
3
/h)、底吹气孔(48孔)位置分布对转炉顶底复吹的影响。结果表明
底吹气孔位置分布是影响熔池搅拌效果的最重要的因素。当选取氧枪距熔池高度h=240mm
顶枪吹气体流量Q
1
=99.0 m
3
/h
底吹气体流量Q
2
=2.4 m
3
/h
底吹气孔(6孔)位置D(4)时
熔池搅拌效果最佳。120 t转炉顶底复吹生产Q235B钢应用结果得出
顶吹流量25 000 m
3
/h
底吹流量560~800 m
3
/h
底吹6孔布置吹炼14~16 min、钢水终点[C
]
0.14%~0.18%
碳氧积0.002 3~0.002 5
熔池搅拌效果良好。
Abstract
Orthogonal experiment with 4 factors and 5 levels by using 120 t BOF geometric similarity 1:7 water model has been earned out to study the effect of height of oxygen lance from pool (200 -280 mm)
top lance flow rate (72. 5 ~ 99. 0 m
3
/h)
bottom blowing flow rate (0. 8 ~2. 4 m
3
/h) and distribution of bottom blowing holes (4 ~ 8 holes) position on BOF top and bottom combined blowing. Results show that distribution of bottom blowing holes position is most important factor to influence the mixing effect of liquid pool
with height of oxygen lance from pool h = 240 mm
top lance flow rate Q
1
=99. 0 m
3
/h
bottom blowing flow rate Q
2
=2. 4 m
3
/h and 6 ho
les bottom blowing position D)(4)
the mixing effect of liquid pool is best. The results of steel Q235B production application of 120 t BOF top and bottom combined blown obtain that with top blowing rate 25 000 m
3
/h
bottom blowing rate 560 ~ 800 m
3
/h and bottom blowing by 6 holes distribution the liquid end [ C
]
is 0. 14% 〜0. 18% and the carbon oxygen product is 0.002 3 ~0.002 5 by blowing for 14 ~ 16 min to get better pool mix effect.