Numerical Simulation on Critical Cooling Rate of Formation of Martensite in High Carbon Steel Rod Coil
|更新时间:2026-01-21
|
Numerical Simulation on Critical Cooling Rate of Formation of Martensite in High Carbon Steel Rod Coil
Special SteelVol. 37, Issue 6, Pages: 9-12(2016)
作者机构:
北京科技大学冶金与生态工程学院,北京,100083
作者简介:
基金信息:
DOI:
CLC:
Received:10 June 2016,
Online First:25 July 2022,
Published:25 July 2016
稿件说明:
移动端阅览
纪元, 李亮, 陆民刚, et al. Numerical Simulation on Critical Cooling Rate of Formation of Martensite in High Carbon Steel Rod Coil[J]. Special Steel, 2016, 37(6): 9-12.
DOI:
纪元, 李亮, 陆民刚, et al. Numerical Simulation on Critical Cooling Rate of Formation of Martensite in High Carbon Steel Rod Coil[J]. Special Steel, 2016, 37(6): 9-12.DOI:
Numerical Simulation on Critical Cooling Rate of Formation of Martensite in High Carbon Steel Rod Coil
By using JMatPro software and according to the 0. 70C steel coil (/%:0. 67C
0. 17Si
0. 50Mn
0. 010P
0. 010S
0. 10Cr) produced at steel works
the effect of C (0. 65% ~ 1. 00% )
Si (0. 20% ~ 0. 55% )
Mn(0. 50% ~ 1. 45%
Cr (0. 10% ~0. 75% )
S (0. 010%~0. 070% )
P (0. 010%~0. 060% ) and austenite grain ratting (5. 0 ~ 8. 0) in high carbon steel rod coil on martensite formation critical cooling rate (CCR
Mf
) has been simulate to get the predict high carbon steel CCR
Mf
expression: CCR
Mf
/(℃·s
-1
) =4. 088 -9
. 98 x [C
]
/% -3.58 x [Si
]
/% -5.12[Mn
]
/% - 0. 001 [P
]
/% +23. 45 x [S
]
/% -7.42 X [Cr
]
/% +2 x G
m
G
m
-austenite grain size rating. Results show that with increasing the C
Mn
Si and Cr content in steel the CCR
Mf
decreases
with increasing the S content in steel and original austenite grain size rating the CCR
Mf
increases and the effect of P on CCR
Mf
is minor; the effect of C and Mn on CCR
Mf
is largest; and the measure value of martensite formation critical cooling rate ( CCR
Mf
) of the 70C steel is 8. 51 ℃/s
and its calculated value is 8. 79℃/s with error 0. 28 ℃/s. It is suggested that during high carbon steel casting process the key point is to control C and Mn segregation and to fine austenite grain size during rolling process for decrease of formation of martensite structure.