Effect of 100 t LF Refining Slag Basicity and Al2O3 Content on Modification and Removal of Inclusions in Steel 65 Mn
|更新时间:2026-01-21
|
Effect of 100 t LF Refining Slag Basicity and Al2O3 Content on Modification and Removal of Inclusions in Steel 65 Mn
Special SteelVol. 38, Issue 4, Pages: 38-42(2017)
作者机构:
作者简介:
基金信息:
DOI:
CLC:
Received:09 February 2017,
Online First:20 July 2022,
Published:20 July 2017
稿件说明:
移动端阅览
刘辉杰, 万勇, 赵和明, et al. Effect of 100 t LF Refining Slag Basicity and Al2O3 Content on Modification and Removal of Inclusions in Steel 65 Mn[J]. Special Steel, 2017, 38(4): 38-42.
DOI:
刘辉杰, 万勇, 赵和明, et al. Effect of 100 t LF Refining Slag Basicity and Al2O3 Content on Modification and Removal of Inclusions in Steel 65 Mn[J]. Special Steel, 2017, 38(4): 38-42.DOI:
Effect of 100 t LF Refining Slag Basicity and Al2O3 Content on Modification and Removal of Inclusions in Steel 65 Mn
With 100 t LF original refining end slag (/% : 53. 8CaO
8. 16MgO
16. 6SiO2
17. 45Al
2
O
3
1. 44TFe
1. 26S
ZG. 08) to improved refining end slag (/% : 51.3CaO
6. 36MgO
25. 0SiO
2
6. 73Al
2
O
3
2. 96TFe
0. 76S
R2. 05) by decreasing the basicity and Al
2
O
3
content in slag
the equivalent number of inclusions in steel 65Mn (/% : 0. 63 ~ 0. 65C
0. 19 ~ 0. 22Si
0. 92 ~ 0. 9
6Mn
0. 005 ~ 0.006S
0. 021 ~ 0. 022P
0.003 5 ~ 0.003 7T [O
]
) decreases from 18. 4 incluisons/mm
2
to 11. 3 inclusions/mm
2
and the average diameter of inclusions reduces from 8. 4 μm to 4.5 μm. As compared with original refining slag by using optimized refining slag the number of Al
2
O
3
per mm
2
in steel 65 Mn at LF end refining decreases from 5. 9 to 1. 7; and the Al
2
O
3
content in CaO-SiO
2
-Al
2
O
3
and CaO-SiO
2
-Al
2
O
3
-MgO compound inclusions decreases from 38. 3% ~ 44. 7% to 17. 5% ~ 28. 7% ; and the reject rate of coil due to unqualified B series Al