Study and Application on Physical Simulation of Single Thick Slab Flow Tundish
|更新时间:2025-10-28
|
Study and Application on Physical Simulation of Single Thick Slab Flow Tundish
Special SteelVol. 43, Issue 1, Pages: 16-21(2022)
作者机构:
1. 本钢板材股份有限公司炼钢厂,本溪,117000
2. 钢铁研究总院国家连铸中心,北京,100081
作者简介:
基金信息:
DOI:
CLC:
Received:25 May 2021,
Online First:09 January 2023,
Published:09 January 2022
稿件说明:
移动端阅览
Jiang Xuefeng, Shi Pengzhao, Wang Yuping, et al. Study and Application on Physical Simulation of Single Thick Slab Flow Tundish[J]. Special Steel, 2022, 43(1): 16-21.
DOI:
Jiang Xuefeng, Shi Pengzhao, Wang Yuping, et al. Study and Application on Physical Simulation of Single Thick Slab Flow Tundish[J]. Special Steel, 2022, 43(1): 16-21.DOI:
Study and Application on Physical Simulation of Single Thick Slab Flow Tundish
In order to obtain a more reasonable 50 t tundish flow control device
a single flow tundish water model with a geometrical similarity ratio of 1:4 is established
and physical simulation tests are carried out to study the effects of different flow rates ( 1.09 and 1.24 m
3
/h )
long nozzle insertion depth(25
50 and 75 mm )
retaining dam height ( 90 and 135 mm )and the distance between long nozzle and weir(190 and 390 mm )on the flow field in tundish. The simulation results show that when the response time is smaller
the dead zone volume of the tundish is larger. The larger the average residence time
the smaller the dead zone volume in tundish. The optimal tundish process parameters of model are: flow control scheme 8
#
flow rate 1. 24 m
3
/h
long nozz
le insertion depth 25 mm
the average residence time is 294. 99 s
the percentage of dead zone volume is 16. 05%. SPHD steel 50 t tundish production application shows that by using flow 40 m