Effect of Controlled Rolling and Cooling Process Parameters on Microstructure of Pipeline Steel X65
|更新时间:2026-01-21
|
Effect of Controlled Rolling and Cooling Process Parameters on Microstructure of Pipeline Steel X65
Special SteelVol. 30, Issue 3, Pages: 55-57(2009)
作者机构:
1. 唐山钢铁股份有限公司技术中心,唐山,063016
2. 唐山科技职业技术学院冶金系,唐山,063001
作者简介:
基金信息:
DOI:
CLC:
Received:27 November 2008,
Online First:24 November 2022,
Published:24 November 2009
稿件说明:
移动端阅览
宋海武, 齐长发, 艾星辉, et al. Effect of Controlled Rolling and Cooling Process Parameters on Microstructure of Pipeline Steel X65[J]. Special Steel, 2009, 30(3): 55-57.
DOI:
宋海武, 齐长发, 艾星辉, et al. Effect of Controlled Rolling and Cooling Process Parameters on Microstructure of Pipeline Steel X65[J]. Special Steel, 2009, 30(3): 55-57.DOI:
Effect of Controlled Rolling and Cooling Process Parameters on Microstructure of Pipeline Steel X65
Effect of cooling rate after rolling (20 ~0. 5 °C /s)
initial pass temperature of finishing rolling ( 1 000 ~ 900 °C )
last pass temperature of finishing rolling (860 ~750 °C ) and coiling temperature (630 ~ 500 °C ) on niicrostnie- ture of pipeline steel X65 (0. 08% C
1. 38% Mn
0. 032% Nb
0. 041 % V
50 x 10
-6
N ) has been studied by using Gleeble-3500 thermal-mechanical simulator. Results showed that with increasing cooling rate after rolling
decreasing reduction ratio at about 950 °C
decreasing finishing and coiling temperature
the microstructure of plate products was finer. The rolling temperature for 7. 1 mm finished plate rolled by 150 mm x 1 700 mm slab was proposed that 1 150 ~ 1 200 °C heating
rough rolling ≤1 130 °C to 35 mm
initial pass finishing rolling 950 ~ 1 020 °C
last pass finishing rolling ≤83O °C
and coiling
≤580 °C
and the mechanical properties of products met the requirement of standard.