Effect of Center Segregation of Hot-Rolled Rod on Mechanical Properties of Oil-Quenched and Tempered Spring Steel 55SiCrA
|更新时间:2026-01-21
|
Effect of Center Segregation of Hot-Rolled Rod on Mechanical Properties of Oil-Quenched and Tempered Spring Steel 55SiCrA
Special SteelVol. 36, Issue 5, Pages: 64-66(2015)
作者机构:
1. 邢台钢铁有限责任公司技术中心,邢台,054027
2. 河北省线材工程技术研究中心,邢台,054027
3. 邢台钢铁有限责任公司炼钢厂,邢台,054027
作者简介:
基金信息:
DOI:
CLC:
Received:13 May 2015,
Online First:16 August 2022,
Published:16 August 2015
稿件说明:
移动端阅览
孟耀青, 郑永瑞, 李拥军, et al. Effect of Center Segregation of Hot-Rolled Rod on Mechanical Properties of Oil-Quenched and Tempered Spring Steel 55SiCrA[J]. Special Steel, 2015, 36(5): 64-66.
DOI:
孟耀青, 郑永瑞, 李拥军, et al. Effect of Center Segregation of Hot-Rolled Rod on Mechanical Properties of Oil-Quenched and Tempered Spring Steel 55SiCrA[J]. Special Steel, 2015, 36(5): 64-66.DOI:
Effect of Center Segregation of Hot-Rolled Rod on Mechanical Properties of Oil-Quenched and Tempered Spring Steel 55SiCrA
The production flowsheet of oil-quenched at 890 ℃ for 300 s and tempered at 530℃ for 1200 s Φ22 mm rod of spring steel 55SiCrA (/% : 0.55C
1.45Si
0.67Mn
0.010P
0.005S
0.68Cr) is hot metal desulphurization- 80 t top and bottom combined blowing converter- LF- RH- 280 mm x 325 mm bloom casting-Φ22 mm rolling products. Examination results show that the center segregation rating of Φ22 mm rolled products of steel 55SiCrA is 3
the carbon content at center of rod is non-homogeneous i. e. 0.50%-0.60% C
and the carbon content at 1/2 radius of rod is 0.54% ; of steel specimen at center the tensile strength is 1430-1455 MPa and the reduction o£ area is 39%-40%
while of steel specimen at 1/2 radius of rod the tensile strength is 1470-1480 MPa and the reduction of area is 43.0%-45.5%
the serious center segregation ( rating 3) leads to obvious decrease of mechanical properties of oil-quenched and tempered spring steel 55SiCrA.