Practice of Quick Desulphurization Technology for Low and Medium Carbon Steel Melting by 70 t EAF-LF

Qin Jun   

  1. Xinjiang Bayi Iron and Steel Co Ltd, Wulumuqi 830022
  • Received:2006-03-01 Online:2006-08-01 Published:2023-03-18

70 t EAF-LF冶炼低、中碳钢快速脱硫的工艺实践

秦 军   

  1. 新疆八一钢铁股份公司板带指挥部,乌鲁木齐830022
  • 作者简介:秦 军(1974),男,高级工程师,1995年重庆大学毕业,从事钢铁冶金工艺生产研究。

Abstract: During 70 t EAF-LF melting steel 20MnSi,the desulphurizing refining time for average sulphur content in steel from 0.060% to 0.015% decreased to 20~30 min from original 30~45 min by adding lime 400~450 kg and synthetic slag 80~250kg,controlling EAF tapping steel temperature 1580~1630℃,increasing refining slag amount, ensuring refining slag basicity 1.5~2.8,Ar stirring rate 180~280  L/min and average(TFe)≤1.0%.

摘要: 在70 t EAF-LF冶炼20MnSi钢过程中,通过EAF出钢时加石灰400~450 kg和合成渣80-250 kg,控制EAF出钢温度1 580~1 630℃,增加精炼渣量,保证精炼渣碱度为1.5-2.8,吹Ar搅拌流量为180~280 L/min, (TFe)平均≤1.0%,可使钢中平均硫含量由0.060%降至0.015%,精炼时间由30~45 min降低至20-30 min。