ISSN:1003-8620

CN:42-1243/TF

Governed by: CITIC Pacific Special Steel Group Co., LTD

Sponsored by: Daye Special Steel Co., LTD.

Special Steel ›› 2006, Vol. 27 ›› Issue (6): 13-14.

Previous Articles     Next Articles

Modelling of Dynamic Recrystallization for a Ti-IF Steel

Xu Guang, Xu Chushao   

  1. College of Material Science and Engineering, Chongqing University, Chongqing 400044
  • Received:2006-04-27 Online:2006-11-01 Published:2023-03-01

Ti-IF钢动态再结晶模型

徐光,徐楚韶   

  1. 重庆大学材料科学与工程学院,重庆400044
  • 作者简介:徐光(1961-),男,教授,系副主任,金属材料加工工艺和 组织性能控制。
  • 基金资助:
    湖北省教育厅重点科研基金资助项目(2002A01010)

Abstract: Single pass reduction deformation experiment of a Ti-IF (interstitial atom free) steel - 0. 009C, 0. 017Si, 0. 13Mn, 0. 012P, 0. 013S, 0. 05Ti, 0. 025Als with deformation rate 0. 1, 1 and 20 s-1 at 750 °C and 850 °C has been carried out by Thermecmastor-Z thermal simulation machine. The curves of work hardening rate - strain for the Ti-IF steel, the dynamic recrystallization diagram and the volume fraction equation of dynamic recrystallization were obtained. Test results show that for the stress-strain curves with no obvious peak strain, it is a available to use work hardening rate method to determine peak strain and stable strain.

Key words:  , Ti-IF Steel, Work Hardening Rate, Peak Strain, Dynamic Recrystallization

摘要: 通过Thermecmastor-Z热模拟实验机对Ti-IF(无间隙原子)钢(%:0.009C、0.017Si、0.13Mn、0.012P、0.013S、0.05Ti、0.025Als)在750℃、850℃和变形速率0.1,1,20s-1下进行单道次压缩变形实验。得出Ti-IF钢加工硬化率-应变曲线、动态再结晶状态图和动态再结晶体积分数方程。实验结果表明,对于无明显峰值应变的应力-应变曲线,采用加工硬化率方法确定峰值应变和稳态应变是一种有效的方法。