ISSN:1003-8620

CN:42-1243/TF

Governed by: CITIC Pacific Special Steel Group Co., LTD

Sponsored by: Daye Special Steel Co., LTD.

Special Steel ›› 2008, Vol. 29 ›› Issue (2): 47-49.

Previous Articles     Next Articles

A Study on Inclusion in Ultra-low Oxygen Spring Steel 60Si2Mn

Zhou Hongxia,Wang Ying and Wang Xinhua   

  1. Metalurgical and Ecological Engineering School,University of Science and Technology,Beijing 100083
  • Online:2008-04-01 Published:2023-01-20

超低氧弹簧钢60Si2Mn的夹杂物研究

周红霞  王  郢  王新华   

  1. 北京科技大学冶金与生态工程学院,北京100083
  • 作者简介:周红霞(1983-),女,北京科技大学在读硕士研究生,从事钢 铁冶炼技术研究。

Abstract: Abstract Spring steel 60Si2Mn produced by 80 tLD-LF(VD)-CC flow sheet using aluminum killing during tap-  ping and aluminum powder strong diffusion deoxidation after tapping to get total oxygen content(T.0)in billet of steel 10×10-6,[S]0.005%,[P]0.010%。Analysis results showed that the main inclusion in steel at end phase of LF and end phase of VD was CaO(MgO)-Al2O3-CaS-SiO2 series,the main inclusion in billet was CaO(MgO)-Al203-CaS-SiO2- TiN compound inclusion. As shielding practice was unsuitable led to increasing[N] and containing TiN inclusion in billet.

Key words: Ultra-low Oxygen Spring Steel,LD-LF(VD)-CC,Al Killing,Inclusion

摘要: 通过80 t LD-LF(VD)-CC流程,采用转炉出钢铝沉淀脱氧,出钢后加铝粉强扩散脱氧工艺所生产的 60Si2Mn弹簧钢铸坯总氧含量(T.0)为10×10-6,[S]0.005%,[P]0.010%。分析结果表明,LF末期和VD末期钢 水中的夹杂物主要为CaO(MgO)-Al203-CaS-Si02系;铸坯中的夹杂物主要为CaO(MgO)-Al203-CaS-SiO2-TiN复合 夹杂。因为连铸时保护浇铸不当,使[N]增加,促使铸坯含TiN夹杂。

关键词: 超低氧弹簧钢LD-LF(VD)-CC Al脱氧夹杂物