ISSN:1003-8620

CN:42-1243/TF

Governed by: CITIC Pacific Special Steel Group Co., LTD

Sponsored by: Daye Special Steel Co., LTD.

Special Steel ›› 2015, Vol. 36 ›› Issue (2): 52-55.

Special Issue: 齿轮钢

Previous Articles     Next Articles

Effect of Hot Deformation Parameters on Grain of Gear Steel Cr14-Co13-Mo5-Ni2

Ge Dong1,2 , Li Jingshe1,2 , Wang Linzhu1,2 , Yang Hongbo1,2 , Yang Shufeng1,2   

  1. 1 School of Metallurgical and Ecological Engineering, 2 State Key Laboratory of Advanced Metallurgy, University of Science and Technology, Beijing 100083
  • Received:2014-10-20 Online:2015-04-01 Published:2022-08-24

热变形参数对Cr14-Co13-Mo5-Ni2齿轮钢晶粒的影响

葛栋1,2,李京社1,2,王林珠1,2,杨宏博1,2,杨树峰1,2   

  1. 北京科技大学1冶金与生态工程学院 ; 2钢铁冶金新技术国家重点实验室,北京 100083;
  • 作者简介:葛栋(1972-),男,博士研究生(北京科技大学),1993年西南科技大学(本科)毕业,钢铁冶金和特殊钢研究。
  • 基金资助:
    国家自然科学基金项目资助(51374021)

Abstract: Test gear steel Cr14-Co13-Mo5-Ni2 is melted by 5 t VIM + 1 t VAR double-vacuum melting process. The effect of deformation temperature (1040-1080 ℃ ),amount of deformation (20%-60% ) and deformation rate (1-20 s-1) on grain distribution and grain size of Cr14-Co13-Mo5-Ni2 steel has been tested and studied by using Gleeble-1500 thermal simulation machine. Results show that with deformation temperature 1040 °C , amount deformation 60% and deformation rate 20 s-1 , the Cr14-Co13-Mo5-Ni2 gear steel has fine, round and homogeneous grain structure, and its average grain size is 4.03 μm.

Key words: Cr14-Co13-Ma5-Ni2 Gear Steel, Thermal Deformation Parameters, Grain Fining, Thermal Simulation

摘要: 试验Cr14-Co13-Mo5-Ni2齿轮钢由5 t VIM+1 t VAR双真空冶炼,利用Gleeble-1500热模拟机试验研究了Cr14-Co13-Mo5-Ni2钢形变温度(1040~1080℃),形变量(20%~60%)和形变速率1~20 s-1对钢的晶粒尺寸的影响。结果表明,形变温度1040℃、形变量60%、形变速率20 s-1时,Cr14-Co13-Mo5-Ni2齿轮钢具有细小圆整均匀的晶粒组织,晶粒平均尺寸为4.03 μm。