Effect of Ti and/or Nb on Structure and Mechanical Properties of High Temperature Alloy 25Cr37Ni0.6Nb

Chen Daofeng1 , Zheng Hongguang2 , Ma Tianjun2 , Shan Aidang1   

  1. 1. School of Material Science and Engineering, Shanghai Jiaotong University, Shanghai 200240 ;
    2. Research Institute, Baoshan Iron and Steel Co Ltd, Shanghai 201900 ;
  • Received:2013-09-17 Online:2014-04-01 Published:2022-09-14

Ti和/或Nb对高温合金25Cr37Ni0.6Nb组织和力学性能的影响

陈道凤1,郑宏光2,马天军2,单爱党1   

  1. 1. 上海交通大学材料科学与工程学院,上海200240;
    2. 宝山钢铁股份有限公司研究院,上海201900;
  • 作者简介:陈道凤(1989-),女,硕士研究生(上海交通大学),2011年华中科技大学(本科)毕业,金属材料研究。

Abstract: The structure and properties of three alloys 0.05C-25Cr-37Ni-0.6Nb(0.6Nb), 0.05C-25Cr-37Ni-0.6Nb-0.6Ti(0.6Nb-0.6Ti) and 0.05C-25Cr-37Ni-l.8Nb( 1.8Nb) melted by 150 kg vacuum induction furnace, rolled to 30 mm plate and solid-solution-treated at 1160-1220 ℃ for 1 h, air cooling have been studied. Results show that as compared with 0.6Nb alloy, the grains in 0.6Nb-0.6Ti alloy added Ti obviously coarsen, the main precipitates are micrometer-scale Ti( CN), the ambient strength and creep behavior at 760 ℃ of 0.6Nb-0.6Ti alloy decrease ; the 1.8Nb alloy got a raise in Nb content the grains fine, the main precipitates are nanometer-scale Nb(CN) , the ambient strength and creep behavior are not obviously changes.

Key words: High Temperature Alloy 25Cr37Ni0.6Nb, Ti, Nb, Solid-Solution Treatment, Precipitates, Grain Coarsening

摘要: 研究了150 kg真空感应炉冶炼并轧成30 mm板的0.05C-25Cr-37Ni-0.6Nb(0.6Nb),0.05C-25Cr-37Ni-0.6Nb-0.6Ti(0.6Nb-0.6Ti)和0.05C-25Cr-37Ni-1.8Nb(1.8Nb)3组合金1160~1220℃ 1 h空冷固溶处理的组织和性能。结果表明,与0.6Nb合金相比加Ti的(0.6Nb-0.6Ti)合金的晶粒明显粗化,析出相主要为微米级Ti(CN),室温强度降低,760℃蠕变性能降低;增加Nb含量的1.8Nb合金的晶粒细化,析出相主要为纳米级Nb(CN),室温强度和蠕变性能没有明显变化。