ISSN:1003-8620

CN:42-1243/TF

Governed by: CITIC Pacific Special Steel Group Co., LTD

Sponsored by: Daye Special Steel Co., LTD.

Special Steel ›› 2012, Vol. 33 ›› Issue (1): 32-34.

Previous Articles     Next Articles

Technology Practice for Ultra-Low-Sulphur Steel Producing by 150 t EAF-LF-VD-CC Flow Sheet

Ma Quanfeng,  Wu Shoufang   

  1. Special Steel Co, Tianjin Pipe Group, Tianjin 300301
  • Received:2011-07-27 Online:2012-02-01 Published:2022-09-20

150 t EAF-LF-VD-CC流程生产超低硫钢的工艺实践

马全峰, 武守防   

  1. 天津钢管集团特钢公司,天津300301
  • 作者简介:马全峰(1968-),男,高级工程师,1991年天津大学毕业,电 弧炉炼钢工艺研究。

Abstract: The production practice shows that for production of 0. 20% 〜0. 24% C ultra-low-sulphur steel, in conditions of 150 t EAF charging- 40% metal + quality low sulphur scrap, EAF end [C] 0. 03% ~0. 05%, EAF tapping average [S] 0. 046%, LF initial average [S] 0. 017%, the ≤0. 001% sulphur content in finishing steel is gotten by controlling refining end [O] ≤2. 5 x 10-6, end ( FeO + MnO) ≤0. 80%, controlling slag amount no less than 22 kg/t and adding aluminium amount 1. 85 kg/t, and sufficient argon stirring.

摘要: 生产超低硫0.20%~0.24%C钢时,在150 t EAF的炉料为40%铁水+优质低硫废钢,终点[C]0.03%~0.05%,电弧炉出钢平均[S]为0.046%,LF初始平均[S]为0.017%的条件下,控制精炼终点[O]≤2.5 X10-6,终点(FeO+MnO)≤O.80%,控制渣量不小于22 kg/t,铝消耗量1.85 kg/t,氩气搅拌良好,成品钢中的硫含量≤0.001%。