An Analysis on Desulphurizing Efficiency during 110 t EBT EAF-LF-RH-CC Process for Production of Seamless Tube Steel 12MnV
|更新时间:2026-01-21
|
An Analysis on Desulphurizing Efficiency during 110 t EBT EAF-LF-RH-CC Process for Production of Seamless Tube Steel 12MnV
Special SteelVol. 32, Issue 2, Pages: 30-33(2011)
作者机构:
1. 北京科技大学冶金生态学院,北京,100083
2. 天津钢管公司,天津,300301
3. 新兴铸管股份有限公司,邯郸,056300
作者简介:
基金信息:
DOI:
CLC:
Received:13 December 2010,
Online First:09 November 2022,
Published:09 November 2011
稿件说明:
移动端阅览
王敬慧, 李京社, 姜桂莲, et al. An Analysis on Desulphurizing Efficiency during 110 t EBT EAF-LF-RH-CC Process for Production of Seamless Tube Steel 12MnV[J]. Special Steel, 2011, 32(2): 30-33.
DOI:
王敬慧, 李京社, 姜桂莲, et al. An Analysis on Desulphurizing Efficiency during 110 t EBT EAF-LF-RH-CC Process for Production of Seamless Tube Steel 12MnV[J]. Special Steel, 2011, 32(2): 30-33.DOI:
An Analysis on Desulphurizing Efficiency during 110 t EBT EAF-LF-RH-CC Process for Production of Seamless Tube Steel 12MnV
The steel 12MnV with ≤0. 003% S is produced by operating such as adding lime in LF
controlling aluminum content at end of LF
injecting 80CaO-20CaF
2
powder in RH process and feeding aluminium wire at end of RH
and feeding calcium-silicon wire after RH process. The desulphurization data show that during the 110 t EAF-LF-RH-CC flow sheet the LF average desulphurizing efficiency is up to 88%
the RH average desulphurizing efficiency is less than 30% ; during steelmaking process for steel deoxidizing by aluminium
in non-feeding aluminium wire condition
with decreasing S content the Al content in steel decreases; and it is favourable for RH desulphurization
as there is sufficient Al in steel to dioxidize before RH process.