A Study on Math Models for Hot Straightening Deformation Resistance and Elastic Modulus of Steel Q345 Medium and Heavy Plate
|更新时间:2026-01-21
|
A Study on Math Models for Hot Straightening Deformation Resistance and Elastic Modulus of Steel Q345 Medium and Heavy Plate
Special SteelVol. 32, Issue 4, Pages: 4-6(2011)
作者机构:
1. 武汉科技大学材料与冶金学院,武汉,430081
2. 武汉钢铁股份有限公司,武汉,430083
作者简介:
基金信息:
DOI:
CLC:
Received:19 January 2011,
Online First:31 October 2022,
Published:31 October 2011
稿件说明:
移动端阅览
谢凯, 程晓茹, 任勇, et al. A Study on Math Models for Hot Straightening Deformation Resistance and Elastic Modulus of Steel Q345 Medium and Heavy Plate[J]. Special Steel, 2011, 32(4): 4-6.
DOI:
谢凯, 程晓茹, 任勇, et al. A Study on Math Models for Hot Straightening Deformation Resistance and Elastic Modulus of Steel Q345 Medium and Heavy Plate[J]. Special Steel, 2011, 32(4): 4-6.DOI:
A Study on Math Models for Hot Straightening Deformation Resistance and Elastic Modulus of Steel Q345 Medium and Heavy Plate
Based on theoretical formulae for medium and heavy plate straightening force and measured data in production of steel Q345 22 〜40 mm plate straightening at 500 ~ 630 T
taking undetermined coefficients in math models of deformation force and elastic modulus as optimized variables
minimum error of straightening force calculation as objective function
the math models of deformation resistance and elastic modulus of steel Q345 medium and heavy plate during straightening process is established by using simplex algorithm to optimized calculate the undetermined coefficients. It is obtained that in straightening process of steel Q345 medium and heavy plate at 500 ~ 630 °C
with increasing temperature (T) the deformation resistance (as) decreases: as = - 1 080. 1 +4. 854 7 T - 0. 004 811 5 尸;and with increasing temperature (T) the elastic modulus (E) increases earlier and decreases later: E = ( -6. 480 7 x 105) + 2 576. 5 T - 2. 387 5 T2. Results show that the relative error between calculated and measured value is less than 5%.