ISSN:1003-8620

CN:42-1243/TF

Governed by: CITIC Pacific Special Steel Group Co., LTD

Sponsored by: Daye Special Steel Co., LTD.

Special Steel ›› 2023, Vol. 44 ›› Issue (3): 29-33.DOI: 10.20057/j.1003-8620.2022-00208

Special Issue: 电炉炼钢

• Process Materials and Development • Previous Articles     Next Articles

Production Practice of 18CrNiMo7-6 Electroslag Process for High-speed Rail Gear Steel

Wang Zhixiang, Nan hai, Zhang Jinwen   

  1. Technology Center , Shangxi Taigang Stainless Steel Co., Ltd., Taiyuan  030003
  • Received:2022-12-22 Online:2023-06-01 Published:2023-05-17

高铁齿轮用钢18CrNiMo7-6电渣生产工艺实践

王之香, 南海, 张锦文   

  1. 山西太钢不锈钢股份有限公司 技术中心,太原 030003
  • 作者简介:王之香(1975-),女,硕士,正高级工程师
  • 基金资助:
    山西省重点研发计划项目(201903D111008)“高铁齿轮钢产品关键生产工艺技术开发及应用”

Abstract: In order to achieve the goal of high cleanliness of high-speed gear steel,especially the size of single-Particle D spherical inclusions ≤10 μm, electroslag process was developed to produce high-speed rail gear steel 18CrNiMo7-6 (/%:0.15-0.21C, ≤0.40Si,0.50-0.90Mn,1.50-1.80Cr,1.40-1.70Ni,0.25-0.35Mo,≤0.010P,≤0.010S),Φ250 mm steel billet production process is EBT electric furnace -LF-VD- casting 5.6 t electrode billet - electroslag remelting - forging - annealing - inspection. The electroslag slag system of 5.6 t electroslag ingot is CaF2∶Al2O3∶CaO∶MgO=65∶20∶10∶5 , in the smelting process the melting rate is controlled at 500-550 kg/h,and the slag amount is 180-200 kg. Compared with the old slag system ,after adopting the new slag system the cleanliness of the produced high-speed gear steel is [O]≤15×10-6, [H]≤1.0×10-6,P≤0.008%,S≤0.005%,and non-metallic inclusion rating of A,B,C ,D and Ds series≤1.0 grade , and the size of single-Particle D spherical inclusions is≤10 μm. Other hardenability and mechanical properties  meet the requirements.

Key words: 18CrNiMo7-6, High-speed Rail Gear steel, Electroslag Remelting, Cleanliness, Hardenability

摘要: 为达到高铁齿轮钢高洁净度,尤其是单颗粒D类球状夹杂物尺寸≤10 μm的目标,开发了电渣工艺生产高铁齿轮用钢18CrNiMo7-6 ( /%:0.15~0.21C,≤0.40Si,0.50~0.90Mn,1.50~1.80Cr,1.40~1.70Ni,0.25~0.35Mo,≤0.010P,≤0.010S ),Ф250 mm钢坯生产工艺流程:EBT电弧炉-LF-VD-模铸5.6 t电极坯-电渣重熔-锻造-退火-检验。采用5.6 t电渣锭,渣系为CaF2∶Al2O3∶CaO∶MgO=65∶20∶10∶5,冶炼过程中熔化率控制在500~550 kg/h,渣量为180~200 kg,采用新渣系后生产高铁齿轮钢的洁净度为[O]≤15×10-6,[H]≤1.0×10-6,P≤0.008%,S≤0.005%,A、B、C、D、DS类非金属夹杂物级别≤1.0级,单颗粒D类球状夹杂物尺寸≤10 μm,淬透性、力学性能等均符合要求。

关键词: 18CrNiMo7-6, 高铁齿轮钢, 电渣重熔, 洁净度, 淬透性